Choose the wrong material for a sulfuric acid pump and the consequences range from accelerated corrosion, shortened seal life, and rising repair bills to a pump-body leak—putting you up against one of the most dangerous chemicals in industry. At Teffiko, we select chemical centrifugal pumps for sulfuric acid service every day. This article compares the sulfuric acid pump materials actually used in engineering, explains the service window and failure mechanism of each, and gives a material-selection framework you can apply directly.


Why There Is No “Universal Material” for Sulfuric Acid

Sulfuric acid is the most-produced industrial chemical in the world, with an annual

output of over 200 million tons; it is widely used in fertilizers, storage batteries,

mining and metallurgy, petroleum refining, and chemical synthesis.

Its corrosion mechanism changes completely with concentration:


  • Dilute to medium concentration (roughly below 65–70%): a strongly reducing acid that continuously attacks the steel surface; the rougher the surface, the faster the corrosion.
  • Concentrated acid (roughly above 80–93%): behaves as a strong oxidizer; it reacts with iron to form a dense ferrous sulfate passivation film that blocks further corrosion.
  • Temperature magnifies every problem. The rule of thumb in corrosion engineering: for every 10°C rise, the corrosion rate roughly doubles. A material acceptable at 25°C may corrode four times faster at 45°C.


Therefore, selection must cover all conditions the pump may encounter—start-up, shut-down, flushing, and process fluctuations—not just the rated design point.

Material 1: Gray Cast Iron and Carbon Steel —Concentrated Acid Only

Service Window

For 80–98% sulfuric acid at ambient temperature, gray cast iron (HT200/HT250) and WCB carbon steel are the standard, most economical choice: the protective layer forms from the acid itself, so no expensive alloy is needed.



  •  Gray cast iron: 80–98% H₂SO₄, 25–50°C
  •  WCB carbon steel: 80–98% H₂SO₄, 25–60°C


Failure Window

The passivation film exists only in strong acid. Below 80% it dissolves; 65–80% is the most dangerous range for iron, where cast iron and carbon steel must never be used. Excessive temperature, high velocity or bubble impingement that damages the film, and water entering the pump and diluting the acid can all break it down. Cast iron must never be used for oleum: free sulfur trioxide reacts with the silicon in cast iron and causes brittle cracking. 



Conclusion: for tightly controlled concentrated-acid tank transfer, this is economical and reliable, but it has almost no margin for concentration or temperature fluctuation. 


Material 2: 316/316L Stainless Steel — The Most Common Selection Trap


316L is the default “chemical-grade” stainless steel—and also the most misused material in sulfuric acid pumps. Its chromium-oxide passivation layer is dissolved by dilute and medium-concentration sulfuric acid, because it lacks the copper and high nickel content needed to resist reducing acids.


316L is acceptable only in an extremely narrow window: 93–100% at ambient temperature, and extremely dilute acid below 5%; it fails rapidly across the 10–90% range.


Conclusion: do not treat 316L as the default material for sulfuric acid pumps; it saves on paper but costs dearly in the field.


Material 3: Alloy 20 (UNS N08020) — The Workhorse for Industrial and Battery Acid


What It Is

Alloy 20 is a nickel-iron-chromium alloy deliberately alloyed with 3–4% copper and 2–3% molybdenum specifically to combat sulfuric acid corrosion. Typical composition: Ni 32–38%, Cr 19–21%, Mo 2–3%, Cu 3–4%, balance iron.


Performance in Service


  •  Concentration: works from about 5% to 98%, with best performance in the 10–70% range, covering most battery acid (29–37%) and process fluids.
  •  Temperature: withstands about 66°C (150°F) at most concentrations.
  •  Velocity: no significant erosion-corrosion at normal in-pump flow velocities.


Limitations and Cost

Above 60–66°C in medium concentrations, corrosion accelerates sharply; high temperature, impurities, or strongly oxidizing fluids exceed its capability. It costs about 3–4 times as much as 316L, but far less than specialty alloys.


Best for: battery acid transfer and circulation, fertilizer acid systems, medium-temperature chemical feed, metal-surface pickling, and acid-cleaning loops.


Material 4: Hastelloy C-276 (UNS N10276) — Top Tier for Severe Service

What It Is

C-276 is a nickel-molybdenum-chromium superalloy (Ni ~57%, Mo 15–17%, Cr 14.5–16.5%, W 3–4.5%) and one of the most corrosion-resistant metal alloys in industry.


Performance in Service


  •  Concentration: covers the full industrial range, including oleum and all medium concentrations.
  •  Temperature: stable to about 120°C (248°F) at many concentrations, far beyond Alloy 20.
  •  Contaminated fluids: resists chlorides, oxidizers, and mixed chemicals that accelerate Alloy 20 corrosion.
  •  High velocity: resists erosion-corrosion and suits high-flow circulation.


Limitations and Cost

The only bottleneck is price: about 5–8 times 316L and 1.5–2.5 times Alloy 20. Where Alloy 20 already suffices, the premium buys no proportional service life.


Best for: hot acid above 60°C, high-temperature concentrated acid, chloride-bearing mixed acids, oleum, high-velocity circulation, and critical production lines where downtime cost far exceeds the alloy premium.


Material 5: PVDF — Fluoropolymer for Purity-First Service


PVDF is a semi-crystalline fluoropolymer in the same family as PTFE, but it can be injection-molded and machined into pump casings and impellers; its carbon-fluorine backbone provides chemical shielding.



  •  Concentration: excellent from dilute acid up to about 70%; above 70% it is attacked and cannot be used.
  •  Temperature: up to about 120°C at low pressure, but its pressure rating drops sharply as temperature rises.
  •  Unique advantages: releases no metal ions into the fluid, weighs far less than metal, and is non-conductive—decisive in battery, semiconductor, and pharmaceutical service.


Limitations: low mechanical strength, creep under long-term load, brittle fracture on impact, and attack by certain organic solvents.

Material 6: PTFE/FEP-Lined Steel Pumps — Steel

When you need fluoropolymer corrosion resistance but cannot accept the pressure limits of an all-plastic pump, a steel casing lined with PTFE or FEP (F46) covers nearly all concentrations and withstands about 80°C.


Two cautions: high temperature and thermal shock cause blistering and delamination of the liner; water ingress locally dilutes the acid, releases heat, and damages the liner. Also, concentrated sulfuric acid has a specific gravity of about 1.84; the motor must be sized for SG 1.84 rather than water, or it will overload.


Side-by-Side Comparison Table


Property Cast Iron / Carbon Steel 316L Alloy 20 C-276 PVDF PTFE/FEP Lined
Optimal Concentration 80–98% Only >93% or <5% 5–98% (best at 10–70%) All ranges, including fuming acid ≤70% Almost all concentrations
Max Temperature 50–60°C Ambient only ~66°C ~120°C ~120°C (low pressure) ~80°C
Dilute / Medium Concentration Not suitable Not suitable Excellent Excellent Excellent Excellent
Concentrated Sulfuric Acid 93–98% Good (low temp) Good (ambient) Good Excellent Not applicable Excellent
Chloride Resistance Poor Poor Moderate Excellent Excellent Excellent
Metal Ion Leaching Yes Yes Yes Yes No No
Relative Cost Lowest Low Medium-high Very high Medium Medium-high
Best Suited For Controlled 98% tank transfer — Battery / industrial acid High temp / contaminated / critical service High purity, ≤70% Wide service range, pressurized

Three-Step Selection Method

1. What is the full concentration range (including the worst case)? If the acid stays below 70% and purity is required, choose PVDF; between 70–98%, choose between Alloy 20 and C-276; for tightly controlled 80–98% ambient-temperature transfer, cast iron/carbon steel remains economical.


2. What is the highest possible temperature? Below 60°C, Alloy 20 covers most conditions; above 60–70°C, or where temperature fluctuations occur, choose C-276.

3. Are chlorides or mixed impurities present? For chloride-bearing service, choose C-276 or a non-metallic solution; Alloy 20's chloride resistance is only moderate. If metal-ion contamination of the product is absolutely unacceptable, only PVDF or a fluoropolymer-lined construction will do.

Do Not Overlook Seals and Gaskets


  •  Mechanical seal faces: prefer SiC/SiC (silicon carbide on silicon carbide) throughout; carbon faces oxidize in concentrated acid.
  •  Secondary seal / bellows: PTFE is the universal safe option; FKM (fluororubber) applies only from dilute to medium concentration and fails in concentrated acid; EPDM and nitrile rubber do not resist sulfuric acid at any concentration.
  •  Springs and small metal parts: use Hastelloy C-276, not 304 stainless steel; acid mist corrodes it and seizes the seal.
  •  Gaskets: use PTFE or expanded PTFE for flanges.   


Common Mistakes

1. Using 316L as the default “chemical-grade” material in the intermediate-concentration range.

2. Exposing cast iron to fluctuating service where concentration may drop below 80%.

3. Selecting material by rated temperature rather than the maximum credible temperature.

4. Ignoring velocity: keep suction below 1.5 m/s and discharge below 3 m/s; high velocity strips off the passivation film.

5. Sizing the motor for water instead of SG 1.84 concentrated acid.

Frequently Asked Questions

What is the best material for a sulfuric acid pump? There is no single answer. For battery and industrial acid below 60°C, Alloy 20 is the most practical; for high temperature, high concentration, contamination, or critical lines, choose C-276; for controlled 80–98% ambient transfer, use cast iron/carbon steel; for high purity or dilute service, choose PVDF or a lined pump.

Can cast iron handle 70% sulfuric acid? No. Below 80% the passivation film dissolves, and 65–80% is most dangerous for iron; switch to a fluoropolymer-lined pump or Alloy 20.

Is C-276 always better than Alloy 20? It resists a wider range, but costs 1.5–2.5 times more. For stable, medium-temperature battery or process acid, Alloy 20 provides adequate life at far lower cost.

Can a lined pump handle 98% sulfuric acid? Chemically, yes. The limits are thermal shock, water ingress, the 80°C temperature ceiling that protects the liner bond, plus a motor sized for SG 1.84.

Conclusion

The best material for a sulfuric acid pump is the one matched to the full concentration and temperature envelope of the acid: cast iron handles controlled concentrated-acid transfer, Alloy 20 handles everyday industrial and battery acid, C-276 handles high temperature and severe service, and PVDF or a lined solution handles purity and broad chemical tolerance.


If your service falls between two materials, or you need to confirm the concentration range, temperature margin, and seal configuration, Teffiko's engineering team can give you a clear wetted-parts, seal, and motor-power package based on your actual operating data. Send Teffiko the concentration, temperature, flow rate, and head, and get a pump proposal with the material confirmed—not a generic catalog quote.



Related News
Leave me a message
  • BACK TO ATHENA GROUP
  • X
    We use cookies to offer you a better browsing experience, analyze site traffic and personalize content. By using this site, you agree to our use of cookies. Privacy Policy
    RejectAccept